Home > PRODUCT > Construction Machinery Wear-Resistant welding wire

RD-152

For buckets, buckets, gears cladding repair

Consultation:

Email: echo_rongda@tuic.net

WhatsApp: +86 13929460585

Product details:

RD-152

——————————————————————————————————————————————

For buckets, buckets, gears cladding repair


Material Characteristics
RD-152 is a bright-arc self-protection wear-resistant flux-cored wire with good overlay performance, beautiful post-weld molding, high strength, high hardness, good abrasion resistance and long service life. The hardness will increase after heat treatment (900℃, 16min, air cooling) of the material after welding.
1.Microstructure: Iron-based high-carbon, high-chromium wear-resistant alloys;Alloy Type: C-Cr-Fe2.Processing performance: only support sanding     
3.Cutting performance: does not support flame cutting4.Surfacing thickness: supports multi-layer surfacing,Overlay thicknesses up to 4-8 mm


Applications

For buckets, buckets, gears cladding repair


Main chemical composition of pure welding layer
C CrMnSiP S Ni MoNb WOthers
0.3-0.4%3.0-4.0%1.0-2.0%1.0-2.0%/
/////≤3.0%
Hardness of pure welding layer                                                          Packaging specification
HRC 50-60                    

15/25/50 KG/Roll

Recommended Surfacing Parameters
Wire Diameter      Current     Voltage  Wire Stick-out Length
1.2/1.6 mm    320-400A    28-31V25-40mm


Welding Precautions

1. When using RD-152 wire, do not use inert gas, and take care to control the current and voltage according to the recommended overlay welding parameters.


2. The overlay layer will have normal fine stress relief cracks, which will help to prevent the occurrence of large-scale spalling of the overlay layer.


3. Before surfacing, please pay attention to removing ash, oil, rust and corrosion in the area to be welded.


4. Oscillating and linear welding are available, can be overlaid with multiple layers, the performance of the alloy layer is related to the dilution rate of the overlaid welding.


5. Preheating can reduce stress cracks.



1.png